Corrosion Inhibition by Polyacrylamide - Zn2+ System for Mild Steel in Simulated Concrete Pore Solution
T. Shanthi1*, S. Sathiyaraj2, S. Rajendran3, J. Sathiyabama4
1*Department of Chemistry, Adhiyaman Arts and Science College for Women, Srinivasa Nagar,
Uthangarai, Krishnagiri (Dt) – India
2PG and Research Department of Chemistry, Jamal Moha Medu College, Trichy, India
3Department of Chemistry, St. Antonys College of Arts and Science for Women, Dindugul – 624005.
4Corrosion Research Centre, PG and Research Department of Chemistry, G.T.N Arts College,
Dindigul- 624 005, India
*Corresponding Author E-mail: shanchem23@gmail.com
ABSTRACT:
The inhibition of corrosion of mild steel immersed in simulated concrete pore solution prepared in well water by polyacrylamide- zinc ion system has been studied using weight–loss, FTIR and AFM methods. Results of weight loss method indicated that inhibition efficiency (IE) increased with increasing inhibitor concentration. The nature of protective film formed on the metal surface has been analysed by FTIR spectra and SEM analysis.
KEYWORDS: Concrete corrosion, simulated concrete pore solution, mild steel, polyacrylamide, well water.
INTRODUCTION:
Corrosion plays a very important role in diverse fields of industry and consequently, in economics. The goal of studying the process of corrosion is to find methods of minimizing to prevent it. Mild steel is widely used as a constitutional material in many industries due to its good mechanical properties of low cost. The corrosion of mild steel is of fundamental academic and industries concern that has received a considerable amount of attention [1-5]. Acid picking paths are employed to remove in desirable scale from the surface of the metals [6-9]. Once the scale is removes the acid is then free for further attack on the metal surface. The use of inhibitors is one of the most practical methods for protection against corrosion especially in acidic media
To evaluate the efficiency of inhibitors in preventing reinforced concrete steel from corrosion there are generally two methods, one uses actual concrete specimens and the other uses the simulated pore solution test, Under normal conditions, reinforcing steel in concrete can be protected from corrosion by forming a compact passive film on its surface in concrete pore solution with high alkalinity (pH 12.5-13.5). However, the passive film can be locally damaged and the localized corrosion of reinforcing steel takes place when pH and/or the chloride concentration at the steel/concrete interface reach the critical values for corrosion [10-15].
Several research papers have investigated the corrosion behaviour of metals in presence of simulated concrete pore (SCP) solutions [16-27]. Usually steel robars have been used in such studies. The present study is undertaken to investigate the corrosion behaviour of three materials, namely, mild steel (MS), galvanized steel (GS) and SS 316L in simulated concrete pore (SCP) solution. A saturated solution of calcium hydroxide is used as SCP solution [28-32].
Polymers, both naturally occurring and synthetic ones, have been studied as metal corrosion inhibitors. Interest in them arose from their stability in acid media, low cost, and the presence of multiple adsorption sites in their molecular structure for bonding with a metal surface. Among those studied to date include polyethylene glycol, polyvinyl alcohol, polyacrylamide, carboxyl methylcellulose, poly (aminoquinone), polyethylene glycol methyl ether (PEGME), polyvinyl pyrrolidone and polyethylenimine, poly (4-vinylpyridne),and poly (diphenylamine)[29–40], to mention but a few.
The present work in undertaken
1. To evaluate the inhibition efficiency of Polyacrylamide-Zn ion in controlling corrosion of mild steel in SCPS prepared in well water
2. To understand the mechanistic aspects of corrosion inhibition and formation of protective film on the metal surface by FTIR and AFM .
METHODOLOGY:
Preparation of Simulated Concrete pore solution (SCPS):
A saturated calcium hydroxide solution is used in present in the present study, as SCP solution. However in numerous studies of rebar corrosion, saturated calcium hydroxide has been used as a substitute for pore solution.
Preparation of the specimens:
Mild steel specimen was used in the present study. (Composition (wt %): 0.026 S, 0.06 P, 0.4 Mn, 0.1 C and balance iron. The dimension of the specimen was1 x 4 x 0.2cm were polished to a mirror finish and degreased with trichloroethylene and used for the weight-loss method and surface examination studies. The environment chosen is well water and the physico-chemical parameter of well water is given in table 1.
Table 1 Physico- chemical parameters of well water
|
Parameters |
Value |
|
pH |
8.38 |
|
Conductivity |
1770μ_-1cm-1 |
|
Chloride |
665 ppm |
|
Sulphate |
214 ppm |
|
TDS |
1100 ppm |
|
Total hardness |
402 ppm |
|
Total Alkalinity |
390 ppm |
|
Magnesium |
83 ppm |
|
Potassium |
55 ppm |
|
Sodium |
172 ppm |
|
Calcium |
88 ppm |
Mass-loss method:
Mild steel specimens in triplicate were immersed in 100 mL of simulated concrete pore solution (SCPS) containing various concentrations of the inhibitor in the presence and absence of Zn2+ for one day. The weight of the specimens before and after immersion was determined using Shimadzu balance, model AY 210. The corrosion products were cleansed with Clarke’s solution. Then the inhibition efficiency (I.E.) was then calculated using the equation(1)
I.E = 100 [1-(W2/W1)] % -------------------------------- (1)
Where W1 and W2 are the corrosion rates in the absence and presence of the inhibitor respectively. The corrosion rate (CR) was calculated using the formula (2).
CR= [(Weight loss in mg) / (Area of the specimens in dm2 x immersion period in days) mdd------------------(2)
Surface Examination study:
The mild steel specimens were immersed in various test solutions for a period of 24 hours . The nature of the film formed on the surface of the metal specimens was analysed for surface analysis technique of FTIR spectra and SEM.
Fourier Transform Infrared Spectra:
FTIR spectra were recorded in a Perkin – Elmer1600spectrophotometer. The film was carefully removed, mixed thoroughly with KBr made into pellets and FTIR spectra were recorded
Scanning electron microscopy:
The mild steel specimens immersed in various test solutions for one day using double distilled water, dried and subjected to the surface examination. The surface morphology measurements of the mild steel surface were carried out by scanning electron microscopy (SEM) using HITACHI –S-3000H SEM.
RESULTS AND DISCUSSION:
Analysis of weight loss study:
The calculated inhibition efficiencies (IE) and corrosion rates (CR) PAA in controlling corrosion mild steel immersed in simulated concrete pore solution in the absence and presense of Zn2+ ion are given in table 2.The calculated value indicates the ability of PAA to be a good corrosion inhibitor PAA alone shows some IE. But the combination of PAA 100 ppm and Zn2+ 50 ppm shows 90% IE.
Table 2 Inhibition efficiencies (IE%) and corrosion rates (CR) obtained from the system, when mild steel immersed in Simulated concrete pore solution prepared in well water
|
System |
IE % |
CR mdd |
|
50 ppm PAA |
60 |
15.6 |
|
100 ppm PAA |
75 |
9.75 |
|
PAA 50 ppm +Zn2+ 50 ppm |
80 |
7.8 |
|
PAA 100 ppm +Zn2+ 50 ppm |
90 |
3.9 |
Surface Analysis:
The protective film formed on the surface of the metal in the presence of PAA- Zn2+ has been analyzed by FTIR spectroscopy.
Analysis of FTIR Spectra:
Scheme -1 : The structure of polyacrylamide
FTIR spectrum of pure PAA is shown in figure 1(a) The –NH stretching and deformation frequencies appear at 3442 cm-1and 1641 cm-1 respectively. The C=O stretching frequency appear at 1650 cm-1 The –CN stretching frequency appears 1021 cm-1. The FTIR spectra of film formed on the metal surface after immersion in solution containing SCPS, 100 ppm of PAA and 50 ppm Zn2+ is shown in figure 1(b). The NH stretching frequency has shifted from 3435cm-1to 3500 cm-1, the NH deformation frequency has shifted from 1641 cm-1 to 1645 cm-1.This observation suggest that PAA has coordinated with Fe2+ through the nitrogen atom NH group resulting in the formation of Fe2+ - PAA complex on the anodic sites of the metal surface. The peak at 1384 is due to Zn-O stretching. The OH stretching frequency appears at 3442 cm-1. This confirms that Zn(OH)2 is formed on the cathodic sites of the metal surface. The CaO stretching frequency appears at 1350 cm-1. The peak at 1470 cm-1 and also COO group is due to CaCo3 stretching. Thus the FTIR spectra study leads to the conclusion that the protective film consists of Fe2+ - PAA complex, CaO and CaCO3 .
(a)
(b)
Figure -1 FTIR Spectrum of (a) Pure PAA (b) Film formed on the metal surface after immersion in aqueous solution containing SCPS+100 ppm of PAA+ 50 ppm of Zn 2+
Scanning electron microscopy:
SEM provides a pictorial representation of the surface. To understand the nature of the surface film in the absence and presence of inhibitors and the extent of corrosion of mild steel, the SEM micrographs of the surface examined. The SEM micrograph of different magnification of polished mild steel surface (Control) in Figure 2(a) shows the smooth surface of the metal. This shows the absence of any corrosion products or inhibitor complex formed on the metal surface. The SEM micrographs of different magnification of mild steel surface immersed in the SCPS for one day is shown in Figure 2 (b) shows the roughness of the metal surface which indicates the highly corroded area of mild steel in SCPS.
The SEM micrographs of different magnification of mild steel surface immersed in the SCPS containing 100 ppm of PAA and 50 ppm of Zn 2+ is shown in Figure 2(c). This shows the rate of corrosion is suppressed,the metal surface is free from corrosion due to the formation of insoluble complex on the metal surface. In the presence of PAA- Zn2+, the surface is covered by a thin layer of inhibitors which effectively control the dissolution of mild steel.
|
(a) |
(b) |
(c) |
|
Figure 2. SEM analysis of a) Polished mild steel (control), b) mild steel immersed in SCPS (Blank) c) mild steel immersed in SCPS + + PAA 50 ppm + Zn2+ 50 ppm |
||
CONCLUSION:
The present study leads to the following conclusion:
1. Inhibition efficiency (IE) of polyacrylamide (PAA) in controlling corrosion of mild steel immersed in simulated concrete pore solution prepared in well water
2. The formulation consisting of 100 ppm PAA and 50 ppm Zn2+ has 90 % corrosion inhibition efficiency.
3. The FTIR spectra reveals that a protective film is formed on the metal surface. The SEM micrographs confirm the formation of protective layer on the metal surface.
ACKNOWLEDGEMENT:
The authors are thankful to their respective management and university grants commission, New Delhi, India,
REFRENCES:
1. F. Bentiss, M. Traisnel, L. Gengembre and M. Lagrene’e, A New Triazole Derivative as Inhibitor of the acid corrosion of mild steel; Electrochemical studies, Weight loss determination, SEM AND XPS, Applied surface science, 152(3-4), 1999, 237-249.
2. F. Bentiss, M. Lagrene’e, M. Traisnel and J. Gorenez, The Corrosion Inhibition of Mild Steel In acidic Media By A New Triazole Derivative, Corrosion Science, 41(4), 1999, 789-803
3. S. Ramesh and S. Rajeswari, Corrosion Inhibition of mild steel in neutral aqueous solution by new Triazole derivatives, Electrochimica Acta, 2004, 49(5), 811-820
4. T. Ouhami, A. Aounti, Y. Abed, B. Hammouti, S. Kertit, A. Ramdani and K. Elkacemi, Corrosion inhibition of Armco Iron in 1M HCl media by new Bipyrazolic derivatives, Corrosion Science, 42(6), 2000, 929-940.
5. A.S. Algaber, E.M. El-Nemna and M.M. Saleh, Effect of Octylphenol polyethylene oxide on the corrosion inhibition of steel in 0.5M H2SO4, Material chemistry and physics, 86(1), 2004, 26-32.
6. V. Branzoi, F. Branzol and M. Baibarae, The inhibition of the corrosion of Armco iron in HCl solutions in the presence of surfactants of the type of N-Alkyl Quaternary Ammonium salts, Materials chemistry and physics, 65(3), 2000, 288-297
7. M.A. Quraishi, R. Sardar and D. Jamel, Corrosion inhibition of mild steel in hydrochloric acid by some Aromatic hydrazides, Materials chemistry and physics, 71(3),2001, 309-313.
8. E.E. Oguzie, C. Unaegbu, C.B.N. Okolue and A.I. Onuchukwa, Inhibition of mild steel corrosion in sulphuric acid using Indigo Dye and Synergistic Halide Additives, Materials chemistry and physics, 84(2-3),2004, 363-368.
9. E.E. Oguzie, G.N. Onuoha and A.I. Onuchukwu, Inhibitory mechanism of mild steel corrosion in 2M sulphuric acid solution by Methylene blue Dye, Materials chemistry and physics, 89(2-3), 2005, 305-311
10. M. Moreno, W. Morris, M.G. Alvarez and G.S. Duffo, Corros. Sci. 46 (2004), p. 2681.
11. V. Kumar, Corros. Rev. 16 (1998), p. 317.
12. M. Maslehuddin, M.M. Al-Zahrani, M. Ibrahim, M.H. Al-Mehthel and S.H. Al-Idi, Constr. Build. Mater. 21 (2007), p. 182
13. R.G. Du, R.G. Hu, R.S. Huang and C.J. Lin, Anal, Chem. 78 (2006), p. 3179.
14. B. Huet, V. L’Hostis, F. Miserque and H. Idrissi, Electrochim. Acta 51 (2005), p. 172.
15. C. Alonso, M. Castellote and C. Andrade, Electrochim. Acta 47 (2002), p. 3469.
16. X. Zhou, H.Y. Yang, F.H. Wang, Corrosion Science and Protection Technology 22 (4), (2010), pp. 343- 347.
17. S. Fajardo, D. M. Bastidas, M. P. Ryan, M. Criado, D. S. McPhail, J.M. Bastidas, Applied Surface Science 256 (21), (2010), pp. 6139-6143.
18. W. Chen, R. G. Du, C-Q. Ye, Y-F. Zhu, C-J. Lin, Electrochimica Acta 55 (20) (2010), pp. 5677-5682.
19. L. Wang, Y-L. Zhao, Tiedao Xuebao. Journal of the China Railway Society 32 (4) (2010), pp. 96-101.
20. C. Chastre, M.A.G. Silva, Engineering Structures 32 (8) (2010), pp. 2268-2277.
21. K. Suh, G. Mullins, R. Sen, D. Winters, Journal of Composites for Construction 14 (4) (2010), pp. 388- 396.
22. J. X. Zhang, H.H. Sun, Y.M. Sun, N. Zhang, Journal of Zhejiang University Science A 11 (5) (2010), pp. 382-388.
23. V.T.N. Dao, P. F. Dux, P.H. Morris, A. H. Carse, ACI Materials Journal 107 (3) (2010), pp. 291-296.
24. P. Ghods, O. B. Isgor, G. A. McRae, G.P. Gu, Corrosion Science 52 (5) (2010), pp. 1649-1659.
25. Y. F. Fan, Z. Q. Hu, Y. Z. Zhang, J. L. Liu, Construction and Building Materials 24 (10) (2010), pp. 1975-1983.
26. A. Kenny, A. Katz, Advanced Materials Research 95 (2010), pp. 69-72.
27. B. Huet, V. L’Hostis, L. Tricheux, H. Idrissi, Materials and Corrosion 61 (2), (2010) pp. 111-124
28. S. R. Allahkaram, M. Khodayari, Anti-Corros. Methods Mater. 55 (2008) 250.
29. M.M. Mennucci, E.P. Banczek, P.R.P. Rodrigues, I. Costa, Cement Concrete Compos, 31 (2009) 418.
30. C.J. Kitowski, H.G. Wheat, Corrosion 53 (1997), p. 216.
31. M.F. Hurley, J.R. Scully, Corrosion 62 (2006) 892.
32. L. Li, A.A. Sagues, Corrosion 60 (2004) p. 195.
33. H. Ashassi-Sorkhabi and N. Ghalebsaz-Jeddi, “Inhibition Effect of Polyethylene Glycol on Corrosion of Carbon Steel in Sulphuric Acid”, Mater. Chem. Phys., 92(2005), p. 480.
34. S. K. Sathiyanarayanan, K. Balakrishnan, S. K. Dhawan, and D. C. Trivedi, “Influence of Poly(aminoquinone) on Corrosion Inhibition of Iron in Acid Media”, Appl. Surf. Sci., 252(2005), p. 966.
35. S. Rajendran, S. P. Sridevi, N. Anthony, and A. J. Amairaj, “Corrosion Behavior of Carbon Steel in Polyvinyl Alcohol”, Anti-Corros. Method Mater., 52(2005), p. 102.
36. C. Jeyaprabha, S. Sathiyanarayanan, K. N. L. Phani, and G. Venkatachari, “Investigation of the Inhibitive Effect of Poly (diphenylamine) on Corrosion of Iron in 0.5M H2SO4 Solutions”, J. Electroanal. Chem., 585(2005), p. 250.
37. Y. Jianguo, W. Lin., V. Otieno-Alego, and D. P. Schweinsberg, “Polyvinylpyrrolidone and Polyethylenimine as Corrosion Inhibitors for the Corrosion of a Low Carbon Steel in Phosphoric Acid”, Corros. Sci., 38(1996), p. 587.
38. Y. Abed, B. Hammouti, F. Touhami, A. Aouniti, S. Kertit, A. Mansri, and K. Elkacemi, “Poly (4-vinylpyrindine) (P4VP) as Corrosion Inhibitors of Armco Iron in Molar Sulphuric Acid Solution”, Bull. Electrochem., 17(2001), p. 105.
39. A. K. Dubey and G. Singh, “Corrosion Inhibition of Mild Steel in Sulphuric Acid Solution by Using Polyethylene Glycol Methyl Ether (PEGME)”, Portugaliae Electrochim. Acta, 25(2007), p. 221.
40. K. S. Khairou and A. El-Sayed, “Inhibition Effect of Some Polymers on the Corrosion of Cadmium in a Hydrochloric Acid Solution”, J. Appl. Polym. Sci., 88(2003), p. 866.
Received on 20.08.2018 Modified on 06.10.2018
Accepted on 10.11.2018 © AJRC All right reserved
Asian J. Research Chem. 2018; 11(6):843-847.
DOI: 10.5958/0974-4150.2018.00148.7